References
1- Excellent / 2 - Satisfactory / 3 - Unsatisfactory
PROD. QUIMICOS | PURO | CARB.GRAFITO | BORNCE | FIB. DE VIDRIO |
---|---|---|---|---|
Acetaldeído |
1
|
1
|
1
|
1
|
Acetona |
1
|
1
|
1
|
1
|
Sulfato de Aluminio |
1
|
1
|
2
|
1
|
Clorato de Amonio |
1
|
1
|
3
|
1
|
Hidroxido de Amonio |
1
|
1
|
3
|
2
|
Anilina |
1
|
1
|
3
|
1
|
Benzeno |
1
|
1
|
1
|
1
|
Acido Borico
|
1
|
1
|
1
|
1
|
Salmuera |
1
|
1
|
1
|
1
|
Bromo (Anhidro) |
1
|
3
|
3
|
2
|
Disulfato de carbono |
1
|
1
|
1
|
1
|
Acido cloroacético |
1
|
1
|
2
|
1
|
Clorobenzeno |
1
|
1
|
1
|
1
|
Cloroformo |
1
|
1
|
1
|
1
|
Acido crónico |
1
|
2
|
3
|
2
|
Acido Cítrico |
1
|
1
|
1
|
1
|
Eter dietílico |
1
|
1
|
1
|
1
|
Etilenglicol |
1
|
1
|
1
|
1
|
Acidos Grasos |
1
|
1
|
1
|
1
|
Clorato Férrico |
1
|
1
|
3
|
1
|
Sulfato Férrico |
1
|
1
|
3
|
1
|
Acido Fluorsilísico |
1
|
2
|
3
|
3
|
Acido Fórmico |
1
|
1
|
1
|
1
|
Freon (Liquido) |
1
|
1
|
1
|
1
|
Acido hidrobórico |
1
|
1
|
3
|
2
|
Acido Muriatico |
1
|
1
|
3
|
2
|
Acido Hidrociánico |
1
|
|||
Acido Hidrofluorito |
1
|
1
|
3
|
3
|
Sol.de Sulfato de H.Acido |
1
|
1
|
3
|
3
|
Maleico |
1
|
1
|
1
|
1
|
Sales de Mercurio |
1
|
1
|
2
|
1
|
Nafta |
1
|
1
|
3
|
2
|
Naftalina |
1
|
1
|
3
|
1
|
Sales de Níquel |
1
|
1
|
1
|
1
|
Acido Nítrico (0-50%) |
1
|
1
|
1
|
1
|
Nitro Benzeno |
1
|
1
|
1
|
1
|
Fenol |
1
|
3
|
3
|
2
|
Acido Fosfórico |
1
|
1
|
1
|
1
|
Acido Ftalico |
1
|
1
|
2
|
1
|
Acido Pícrico |
1
|
1
|
1
|
1
|
Piridina |
1
|
1
|
1
|
1
|
Acido Salicilico |
1
|
2
|
3
|
2
|
Nitrato de Plata |
1
|
1
|
1
|
1
|
Carbonato de Sodio |
1
|
1
|
1
|
1
|
Hidróxido de Sodio |
1
|
1
|
1
|
1
|
Nitrato de Sodio |
1
|
1
|
1
|
1
|
Peróxido de Sodio |
1
|
1
|
3
|
1
|
Silicato de Sodio |
1
|
1
|
3
|
1
|
Sulfato de Sodio |
1
|
2
|
3
|
3
|
Acido Sulfúrico |
1
|
1
|
1
|
1
|
Acido Tánico |
1
|
1
|
3
|
2
|
Acido Tartárico |
1
|
1
|
3
|
2
|
Tricloroetileno |
1
|
1
|
3
|
3
|
Clorato de Zinc |
1
|
1
|
3
|
3
|
TECHINCAL FEATURES
P/15 GL
85% VIRGIN PTFE
85% VIRGIN PTFE
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE FF HD | GRADE E | |
---|---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,21 +/- 0,02 | 2,21 +/- 0,02 | 2,21 +/- 0,02 | 2,21 +/- 0,02 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 25 | 22 | 20 | 19 | |
Elongation* | ASTM D 4894 | % | 300 | 280 | 260 | 230 | |
Bulk Density | ASTM D 4894 | g/l | - | 600-700 | 700-800 | 650-750 | |
Hardness | NEEDLE | Shore D | 64 - 60 | 64 - 60 | 64 - 60 | 64 - 60 | |
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,5 | 2,0+/-0,5 | 2,0+/-0,5 | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | 6 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | 6 | |
Average particle size | ISO 13320 | μm | - | 400 - 700 | 400-600 | 400-800 |
RECOMMENDED MOULDING PRESSURE: | 300-4000 Kg/cm² |
MAX SINTERING TEMPERATURE: | 370-375 °C |
GENERAL APPLICATION:
This grade offers a good wear and excellent chemical resistance.
Safety- Toxicology
Technical Information
This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/25 GL
75% VIRGIN PTFE
25% +/-2 GLASS FIBRE
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE FF HD | GRADE EH | ||
---|---|---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,24 +/- 0,02 | 2,24 +/- 0,02 | 2,24 +/- 0,02 | 2,24 +/- 0,02 | ||
Tensile Strenght* | ASTM D 4894 | Mpa | 23 | 20 | 20 | 18 | ||
Elongation* | ASTM D 4894 | % | 270 | 250 | 230 | 200 | ||
Bulk Density | ASTM D 4894 | g/l | - | 600-700 | 650-750 | 700 | ||
Hardness | NEEDLE | Shore D | 66 - 63 | 66-63 | 66-63 | 66-63 | ||
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,5 | 2,0+/-0,5 | 2,0+/-0,5 | - | ||
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | 3 | ||
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | 3 | ||
Average particle size | ISO 13320 | μm | - | 400-700 | 400-600 | 400-700 | ||
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-500 Kg/cm² |
MAX SINTERING TEMPERATURE: | 370-375 °C |
GENERAL APPLICATION:
This grade offers a good wear and excellent chemical resistance. For bearing applications is considered to have optimum glass content and is recommended where contact with hydrochloric acid is involved.
Safety- Toxicology
Technical Information
This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/15 GL 5 MOS
80% VIRGIN PTFE
15% +/- 1 GLASS FIBRE
5 % +/- 0,5 Molybdenum Disulfide
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE EH | |
---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,27 +/- 0,02 | 2,27 +/- 0,02 | 2,27 +/- 0,02 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 24 | 22 | 20 | |
Elongation* | ASTM D 4894 | % | 280 | 250 | 220 | |
Bulk Density | ASTM D 4894 | g/l | - | 700 | 700 | |
Hardness | NEEDLE | Shore D | 65 - 63 | 65-63 | 65-63 | |
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,5 | 2,0+/-0,5 | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | |
Average particle size | ISO 13320 | μm | - | 400-700 | 400-700 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 350-400 Kg/cm² |
MAX SINTERING TEMPERATURE: | 365-370 °C |
GENERAL APPLICATION:
This compound has a high temperature stability (dimensional stability) and high pressure resistance. Reduced cold flow and an increment in the dielectric properties. Good chemical resistance against organic solvents. The MoS2 content reduces friction and abrasion of the metal counterpart. Not suitable for soft metal counterparts. Limitation for hot water usage.
Safety- Toxicology
Technical Information
This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/23 CAR 2 GR
75% VIRGIN PTFE
23% +/- 2 CARBON COKE
2 % +/- 0,2 GRAPHITE POWDER
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE EH | |
---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,09 +/- 0,03 | 2,09 +/- 0,03 | 2,09 +/- 0,03 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 22 | 20 | 18 | |
Elongation* | ASTM D 4894 | % | 120 | 100 | 80 | |
Bulk Density | ASTM D 4894 | g/l | - | 600 | 600 | |
Hardness | NEEDLE | Shore D | 65 - 68 | 65-68 | 65-68 | |
Diametric Shrinkage | INTERNAL | % | 2,5+/-0,5 | 2,5+/-0,5 | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 6 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 6 | |
Average particle size | ISO 13320 | μm | - | 400-700 | 400-800 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-500 Kg/cm² |
MAX SINTERING TEMPERATURE: | 370-375 °C |
GENERAL APPLICATION:
It is preferable to other grades for application involving hydrofluoric acid. It has a higher wear rate. It has proved successfully as piston rings material, particularly in oil-free compressors. The graphite powder content reduces friction and improves the physical properties.
Safety- Toxicology
Technical Information
Technical Information This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/20 GL 5 GR
75% VIRGIN PTFE
20% +/- 1 GLASS FIBRE
5 % +/- 0,5 GRAPHITE POWDER
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE FF HD | GRADE EH | |
---|---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,22 +/- 0,03 | 2,22+/- 0,03 | 2,22 +/- 0,03 | 2,22 +/- 0,03 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 20 | 18 | 18 | 16 | |
Elongation* | ASTM D 4894 | % | 270 | 250 | 200 | 200 | |
Bulk Density | ASTM D 4894 | g/l | - | 600 | 650 | 650 | |
Hardness | NEEDLE | Shore D | 65 - 61 | 65-61 | 65-61 | 65-61 | |
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,5 | 2,0+/-0,5 | 2,0+/-0,5 | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | 3 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | 3 | |
Average particle size | ISO 13320 | μm | - | 400-600 | 400-500 | 400-600 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-500 Kg/cm² |
MAX SINTERING TEMPERATURE: | 370-375 °C |
GENERAL APPLICATION:
This compound offers a good wear and excellent chemical resistance. Graphite content reduces friction.
Safety- Toxicology
Technical Information
Technical Information This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents. .P/40 BZ
60% VIRGIN PTFE
40% +/- 2 IRREGULAR BRONZE POWDER ANTI-OXIDANT
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE FF HD | GRADE E | |
---|---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 3,10 +/- 0,05 | 3,10+/- 0,05 | 3,10 +/- 0,05 | 3,10 +/- 0,05 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 26 | 24 | 22 | 20 | |
Elongation* | ASTM D 4894 | % | 280 | 250 | 240 | 230 | |
Bulk Density | ASTM D 4894 | g/l | - | 980 | 1000 | 950 | |
Hardness | NEEDLE | Shore D | 68 - 64 | 68-64 | 68-64 | 68-64 | |
Diametric Shrinkage | INTERNAL | % | 2,5+/-0,5 | 2,5+/-0,5 | - | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | 6 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | 6 | |
Average particle size | ISO 13320 | μm | - | 400-700 | 400-600 | 400-800 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-600 Kg/cm² |
MAX SINTERING TEMPERATURE: | 365-370 °C |
GENERAL APPLICATION:
Generally recommended as a good bearing material and preferable to glass fibre either at higher speeds, where its greater thermal conductivity is used.
Safety- Toxicology
Technical Information
Technical Information This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/60 BZ
60% +/- 2 IRREGULAR BRONZE POWDER ANTI-OXIDANT
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE E | |
---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 3,9 +/- 0,1 | 3,9+/- 0,1 | 3,9 +/- 0,1 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 22 | 20 | 14 | |
Elongation* | ASTM D 4894 | % | 200 | 180 | 130 | |
Bulk Density | ASTM D 4894 | g/l | - | 1300 | 1300 | |
Hardness | NEEDLE | Shore D | 70 - 66 | 70-66 | 70-66 | |
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,4 | 2,0+/-0,4 | - | |
Flow | INTERNAL | Sec/50 g | - | 3 | 6 | |
Flow stability | INTERNAL | Sec/50 g | - | 3 | 6 | |
Average particle size | ISO 13320 | μm | - | 700-400 | 800-400 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-600 Kg/cm² |
MAX SINTERING TEMPERATURE: | 365-370 °C |
GENERAL APPLICATION:
Generally recommended as a good bearing material and preferable to glass fibre either at higher speeds, where its greater thermal conductivity is used.
Safety- Toxicology
Technical Information
This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/55 BZ 5 MOS
45% VIRGIN PTFE
55% +/- 2 IRREGULAR BRONZE POWDER ANTI-OXIDANT
5% +/- 0,5 MOLIBDENUM DISULPHIDE (MoS2)
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | |
---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 3,85 +/- 0,03 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 20 | |
Elongation* | ASTM D 4894 | % | 130 | |
Bulk Density | ASTM D 4894 | g/l | - | |
Hardness | NEEDLE | Shore D | 72 - 68 | |
Diametric Shrinkage | INTERNAL | % | 2,0+/-0,5 | |
Flow | INTERNAL | Sec/50 g | - | |
Flow stability | INTERNAL | Sec/50 g | - | |
Average particle size | ISO 13320 | μm | - | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 400-500 Kg/cm² |
MAX SINTERING TEMPERATURE: | 360-365 °C |
GENERAL APPLICATION:
Sealing for automatic gear boxes. This compound has the highest pressure resistance and the lowest abrasion of seals and counterparts.
Safety- Toxicology
Technical Information
This information is based on our experience to date and we believe it to be reliable. It is intended only as a guide for use at your discretion and risk. We cannot assume liability in connection with the final use or transformation of the products described in this TDS. None of this information is to be taken as a licence to operate under, in order to infringe any patents.P/15 GR
85% VIRGIN PTFE
15% +/- 1 GRAPHITE POWDER
MECHANICAL PROPERTIES | TEST METHOD | UNITS | GRADE NFF | GRADE FF | GRADE FF HD | GRADE EH | |
---|---|---|---|---|---|---|---|
Specific gravity | ASTM D 4894 | g/cm3 | 2,16 +/- 0,02 | 2,16 +/- 0,02 | 2,16 +/- 0,02 | 2,16 +/- 0,02 | |
Tensile Strenght* | ASTM D 4894 | Mpa | 23 | 20 | 18 | 16 | |
Elongation* | ASTM D 4894 | % | 250 | 200 | 180 | 140 | |
Bulk Density | ASTM D 4894 | g/l | - | 600 | 700 | 650 | |
Hardness | NEEDLE | Shore D | 60 - 63 | 60 - 63 | 60 - 63 | 60 - 63 | |
Diametric Shrinkage | INTERNAL | % | 2,5+/-0,5 | 2,5+/-0,5 | 2,5+/-0,5 | - | |
Flow | INTERNAL | Sec/50 g | - | 4 | 3 | 4 | |
Flow stability | INTERNAL | Sec/50 g | - | 4 | 3 | 4 | |
Average particle size | ISO 13320 | μm | - | 400-700 | 400-600 | 400-700 | |
* Cross direcction |
RECOMMENDED MOULDING PRESSURE: | 300-350 Kg/cm² |
MAX SINTERING TEMPERATURE: | 370-375 °C |
GENERAL APPLICATION:
This compound is used against aggressive and corrosive agents. It is used in hot water and steam application. It has a good heat conductivity. It has permission for usage in food application. The wear characteristics approximately 5 times better than virgin PTFE. Low coefficient of friction compared to GL/CAR/BZ compounds. Low abrasion when used against soft metals counterparts. Low hardness compared to standard compounds as GL/CAR/BZ etc.